Viscometry

Falling Ball Viscometry: The falling ball viscometry method[8] is the oldest and simplest viscometry method. In this method, the time for the ball to fall a known distance in the fluid is measured and the terminal velocity u is determined from which a viscosity can be calculated. Assuming Newtonian behaviour the apparent viscosity h which depends on the densities of the ball and fluid Á b and Á f, respectively and the radius R of the ball and gravitational constant g:

The falling ball viscometer can be sealed to prevent evaporation or even to permit measurements at high pressure. However, to avoid complex flow patterns there must be a significant gap between the falling ball and the wall, which limits the method to materials that have a reasonable degree of transparency. The range of strain rates that can be covered is low. This method is not particularly suitable for rate-dependent, visco-elastic materials such as adhesives.

A variation on the falling ball method is the rolling ball method[9] where the tube is inclined at known angles and the velocity of the rolling ball measured. As the ball is in contact with the wall even opaque liquids can be measured. Varying the angle of incline allows variation in the shear stress and shear rate. However, analysis of the flow is much more complex. The falling or rolling ball technique is well suited for quality control applications, as changes in viscosity ought to be apparent through changes in “time of flight.”

Hydrostatic Head Viscometers: Hydrostatic head viscometers rely on the pressure generated by the fluid mass to provide driving force for flow. The simplest techniques use flow cups [3] in which the adhesive is placed into a vessel with a drain hole and the rate at which the adhesive flows from the cup is measured, as described above. This gives a qualitative value for the relative viscosities of different materials.

Hydrostatic head (‘U’ tube) viscometers: (a) Ostwald; (b) Ubbelohde; and (c) reverse flow

The Ostwald, Ubbelohde and reverse flow hydrostatic head viscometers are the most popular for general and high precision measurement of the viscosity of thin Newtonian fluids. The time for the fluid to fall or rise between marks A and B (which is proportional to the kinematic viscosity) determines the flow rate Q. The pressure drop DP is calculated from the head of fluid. The viscosity can be determined from these values and the geometry of the viscometer. The use of tube viscometers such as these is covered in various standards [4–6]. These relatively cheap, easy to use viscometers are capable of high reproducibility and repeatability.

However, the pressure drops are low. Measurement of the rheology of thick, paste adhesives would be problematic, if not impossible, using such instruments. A further limitation of these types of viscometers is that they are not suitable for measuring the viscosity of non-Newtonian fluids. There are insufficient ranges of shear stress and shear rates available for the measurement of fluids exhibiting behaviour of this nature. For these reasons, hydrostatic head viscometers are unsuitable for the majority of adhesives with the exception of thin liquid adhesives, such as cyanoacrylates or anaerobics.

Next: Capillary Rheometers